Interpretation of the performance indicators of carbon raisers
Fixed carbon content, ash content, particle size, and other factors affect carbon absorption rate, while sulfur content, nitrogen content, volatile matter, and moisture content directly lead to casting defects.

Particle Size Distribution
The particle size distribution of graphitized recarburizers can be measured using a laser particle size analyzer to determine the proportion of different particle size ranges, average particle size, and maximum particle size. The particle size of the recarburizer should be selected based on the melting method, furnace type, and furnace size. For example, for induction furnaces, the particle size range is 0.2–6 mm; for steel and other ferrous metals, the particle size range is 1.4–9.5 mm; for high-carbon steel requiring low nitrogen content, the particle size range is 0.5–5 mm. The specific choice should be determined based on the furnace type, the type of workpiece being melted, and other details. Additionally, particle uniformity should be ensured, as uneven particle size is one of the reasons for poor absorption efficiency. To improve carbon absorption, recarburizers should undergo particle size treatment to remove fine powders and coarse particles.

Moisture Content
The total moisture content of the recarburizer should be as low as possible, as moisture introduced into molten steel increases the hydrogen content in the steel. The total moisture content depends on the coke quenching process, storage, and transportation conditions. The moisture content of small-bag recarburizers should be ≤1%, while the moisture content of raw coke before crushing and packaging should be ≤3%.
Ash Content and Fixed Carbon Content
The fixed carbon content of a recarburizer represents its truly useful portion, and a higher value is better. Fixed carbon cannot be directly measured but is a calculated value. The lower the ash and volatile matter content of the recarburizer, the higher the fixed carbon content.
Fixed carbon and ash content are opposing parameters in recarburizers, and they are the two most important factors affecting carbon absorption efficiency. Recarburizers with high fixed carbon content and low ash content yield high carbon absorption efficiency, while the opposite results in low efficiency.
Recarburizers with high ash content are prone to "coking," forming a slag layer that isolates carbon particles and prevents them from dissolving, thereby reducing carbon absorption. Additionally, they increase the amount of slag, prolong operation time, increase power consumption, and add to the labor required during the melting process. When using channel induction furnaces, if recarburizers are added to the furnace, low-ash varieties should be chosen to prevent oxides from accumulating in the channels and affecting electrical efficiency.
The ash content varies significantly among different types of recarburizers. Graphite recarburizers have relatively low ash content, around 0.5–1.0%, while calcined anthracite has higher ash content, with even high-quality ones not falling below 4–5%.
From the perspective of carbon absorption efficiency, higher fixed carbon content and lower ash content are desirable. However, production costs and the impact on molten iron quality must also be considered.
Volatile Matter Content
Volatile matter is an ineffective component of recarburizers. When volatile matter enters molten steel, it increases the gas content in the molten iron, raising the risk of porosity defects in castings. The volatile matter content depends on the calcination or coking temperature and the treatment process of the recarburizer. Properly treated recarburizers have a volatile matter content below 0.5%. Therefore, anthracite and raw petroleum coke should not be used as recarburizers.
Calcined anthracite, calcined petroleum coke, and synthetic graphite undergo high-temperature treatment, resulting in very low volatile matter and moisture content. As such, these parameters are generally not tested or considered as key factors.

Sulfur Content
Sulfur in recarburizers is a harmful element that reduces the ductility and toughness of steel; the lower the sulfur content, the better. The sulfur content of a recarburizer depends on the sulfur content of the raw material and the calcination temperature.
Sulfur is a harmful element that interferes with spheroidization. For nodular cast iron, the sulfur content in the base molten iron is generally required to be ≤0.015%, so recarburizers used for nodular cast iron should have as low a sulfur content as possible. For gray cast iron, to ensure effective inoculation, the sulfur content in the molten iron is generally required to be 0.06–0.12%, so recarburizers for gray cast iron can tolerate higher sulfur content.
Nitrogen Content
The nitrogen content in recarburizers has a dual effect in gray cast iron. It is generally believed that when nitrogen content is between 70 and 120 ppm, nitrogen stabilizes pearlite, bends flake graphite, and blunts its tips, thereby improving the mechanical properties of gray cast iron. However, when the nitrogen content in gray cast iron exceeds the equilibrium concentration (generally considered to be around 140 ppm), the casting is prone to fissure-type nitrogen porosity defects. Therefore, selecting a recarburizer with an appropriate nitrogen content is critical.
For gray cast iron, coal-based or petroleum coke recarburizers are commonly chosen, with a nitrogen content of around 1000 ppm meeting the requirements of most casting materials. For nodular cast iron, graphite recarburizers or graphitized recarburizers are required.